MATERIALS — 6063-T5
Materials
6063-T5 aluminum billet, three-axis CNC machining, and the finishing process behind every Torque case.
We looked at 7075 early on — it's stiffer and the alloy of choice for a lot of enthusiast keyboard cases — and moved off it once we timed how long it took the Anvil to rough a case out of it. 7075 machines slower, dulls tooling faster, and the stiffness advantage doesn't matter much in a part that isn't load-bearing the way an aircraft bracket is. 6063-T5 cuts fast, holds a tight tolerance, anodizes evenly, and lets us keep cycle times low enough to hit forty boards a week on one mill.
The billet
Every case starts as a 1.4-kilogram bar of 6063-T5, extruded and pre-aged to its final temper before it reaches the shop — T5 means it's been artificially aged straight from the extrusion process rather than solution heat-treated afterward, which keeps the material stable and consistent bar to bar. Bars arrive in six-meter lengths and get cut to rough blanks on a band saw before anything touches the mill.
| Property | Value |
|---|---|
| Alloy | 6063 |
| Temper | T5 |
| Tensile strength | ~215 MPa |
| Starting blank | 1.4kg |
| Finished case | ~450g |
Machining
A blank is faced, drilled, and fixtured, then the Anvil — our three-axis mill, older than the company and rebuilt twice — runs a roughing pass followed by a finishing pass, about fifty-five minutes total per case. The plate-mounting holes, the switch cutouts, and the USB-C port opening are all cut in the same setup, which is what keeps them registered to each other within ±0.02mm; a second setup would mean a second reference point and a wider tolerance stack.
| Feature | Tolerance |
|---|---|
| Plate mounting holes | ±0.02mm |
| Switch plate cutouts | ±0.05mm |
| Overall case dimensions | ±0.1mm |
| Screw boss depth | ±0.03mm |
Finishing
After machining, cases go through a bead-blast cabinet that gives the aluminum its matte, fingerprint-resistant surface, then into a Type II anodizing tank. Anodizing grows a layer of aluminum oxide directly out of the surface rather than coating over it, so the finish can't chip or peel the way paint would — it can scratch through to bare metal under enough abrasion, but it won't flake.
Clean a case with a barely damp microfiber cloth and, if needed, a drop of isopropyl alcohol for fingerprints. Skip ammonia-based glass cleaners — they can dull an anodized finish over repeated use — and never submerge a board; the switches and PCB underneath are not sealed.
Weight and waste
A finished TQ-75 case weighs 780g, down from a 1.4kg blank — better than two-thirds of the material is removed as swarf over the course of machining. That swarf is bagged by alloy and returned to the same supplier who sold us the billet, where it's re-melted into new extrusion stock rather than sold off as scrap to a generic recycler. It isn't a closed loop, but it's a shorter one than most.
Revision dated September 12, 2025